Chinese-made American standard steel plate grades ASTM A516 Grade 65 Chemical composition of pressure vessel plates&Mechanical properties
ASTM A516 Grade 65 Approaching Steel Plate Grade Lookup Table
| Grade | Chemical composition | Mechanical properties | Remark | |||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| C ① ② Thickness (mm) | Mn ② Thickness(mm) | Si | S ① | P ① | Ni | … | ReH ③ | Rm | KV₂ | A% Gauge length 50mm ④ | A% Gauge length 200mm ④ | |||||||||||||||||||||||||||||||||||||||||||||||||
| ASTM A516 Grade65 | ≤12.5mm | 12.5~50mm | 50~100mm | 100~200mm | >200mm | ≤ 12.5mm | >12.5mm |
SA 0.15~0.40 |
FA 0.13~0.45 |
≤0.025 | ≤0.025 | ≥240 | 450~585 | ≥23 | ≥19 | |||||||||||||||||||||||||||||||||||||||||||||
| ≤0.24 | ≤0.26 | ≤0.28 | ≤0.29 | ≤0.29 |
SA 0.85~1.20 |
FA 0.79~1.30 |
FA 0.85~1.20 |
FA 0.791.30 |
||||||||||||||||||||||||||||||||||||||||||||||||||||
Notes:
Smelting Analysis=SA
Finished Product Analysis=FA
①:Applicable to both smelting analysis and finished product analysis.
②:For every 0.01% decrease below the specified maximum carbon content, the upper limit of the specified maximum manganese content can be increased by 0.06%, with a maximum allowable limit of 1.50% for smelting analysis and a maximum allowable limit of 1.60% for finished product analysis.
③:Determined by the 0.2% residual deformation method or the 0.5% elongation under load.
④:For corrections regarding elongation, see standard A-20/A20M.