Product Uses and Introduction
This series of products is for wind power applications, and the material selection needs to be determined based on the specific circumstances. Below, we will introduce the thickness range, delivery status, and applicable standards for each grade that we can provide. We hope this information is helpful. If you have any questions about the products or need a quote, please contact us via email. Because some grades can be categorized into multiple types according to their applications, this may cause some inconvenience in your search, for which we sincerely apologize. We also welcome any suggestions you may have. Thank you very much!
Spot inventory inquiry Spot inventoryIf conditions permit, we can also provide steel mill customization services, where the thickness, width, and length can all be made to your needs, just like a tailor making clothes for you, implementing personalized orders.
Steel mill customized business email: customize@cehesteel.com
Scope of supply
| Grade | Thickness(mm) | Delivery status | Ordering Standards | Remarks | ||||||||||||||||||
| Q345C/D/E | 6~100 | AR、CR、TM、NR、N | GB/T1591 | All steel grades can be produced according to GB/T5313 , including Z-axis plates (Z15, Z25, Z35).with a minimum thickness of 15mm. |
||||||||||||||||||
| Q355C/D | 6~100 | AR、CR | GB/T1591 | |||||||||||||||||||
| Q355NC/D/E | 6~100 | NR、N | GB/T1591 | |||||||||||||||||||
| Q355MC/D/E | 6~60 | TM | GB/T1591 | |||||||||||||||||||
| Q345FTC/D/E | 6~100 | AR、CR | GB/T 28410 | |||||||||||||||||||
| 6~100 | NR、N | GB/T28410 | ||||||||||||||||||||
| 6~60 | TM | GB/T 28410 | ||||||||||||||||||||
| GB/T712 DH36/EH36 | 6~60 | TM | GB/T712 | |||||||||||||||||||
| GB/T712 DH36/EH36 | 6~80 | N | GB/T712 | |||||||||||||||||||
| S355JR/J0/J2/K2 | 6~100 | AR、CR、N | EN 10025-2 | |||||||||||||||||||
Chemical Composition
| Grade | Quality grade | Chemical Composition/% | ||||||||||||||||||||||||||||||
| C | Mnᵃ | P | S | Si | Nb | V | Ti | Mo | Cr | Ni | Cu | Als | N | |||||||||||||||||||
| ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≤ | ≥ | ≤ | ||||||||||||||||||||
| Q235FT | B、C | 0.18 | 0.50~1.40 | 0.030 | 0.025 | 0.50 | 0.050 | 0.060 | 0.050 | 0.10 | 0.30 | 0.30 | 0.30 | 0.015 | 0.012 | |||||||||||||||||
| D、E | 0.025 | 0.020 | ||||||||||||||||||||||||||||||
| Q275FT | C | 0.18 | 0.50~1.50 | 0.025 | 0.020 | 0.50 | 0.050 | 0.060 | 0.050 | 0.10 | 0.30 | 0.30 | 0.30 | 0.015 | 0.012 | |||||||||||||||||
| D | 0.015 | |||||||||||||||||||||||||||||||
| E、F | 0.010 | |||||||||||||||||||||||||||||||
| Q345FT | C、D | 0.20 | 0.90~1.65 | 0.025 | 0.015 | 0.50 | 0.06 | 0.12 | 0.050 | 0.20 | 0.30 | 0.50 | 0.30 | 0.015 | 0.012 | |||||||||||||||||
| E、F | 0.020 | 0.010 | 0.010 | |||||||||||||||||||||||||||||
| Q420FT | C、D | 0.20 | 1.00~1.70 | 0.025 | 0.015 | 0.50 | 0.06 | 0.15 | 0.050 | 0.20 | 0.30 | 0.50 | 0.30 | 0.015 | 0.012 | |||||||||||||||||
| E、F | 0.020 | 0.010 | 0.010 | |||||||||||||||||||||||||||||
| Q460FT | C、D | 0.20 | 1.00~1.70 | 0.025 | 0.015 | 0.60 | 0.07 | 0.15 | 0.050 | 0.30 | 0.60 | 0.80 | 0.55 | 0.015 | 0.012 | |||||||||||||||||
| E、F | 0.020 | 0.010 | 0.010 | |||||||||||||||||||||||||||||
| Q550FT | D | 0.20 | ≤1.80 | 0.020 | 0.010 | 0.60 | 0.07 | 0.15 | 0.050 | 0.50 | 0.80 | 0.80 | 0.80 | 0.015 | 0.012 | |||||||||||||||||
| E | 0.010 | |||||||||||||||||||||||||||||||
| Q620FT | D | 0.20 | ≤1.80 | 0.020 | 0.010 | 0.60 | 0.07 | 0.15 | 0.050 | 0.50 | 0.80 | 0.80 | 0.80 | 0.015 | 0.012 | |||||||||||||||||
| E | 0.010 | |||||||||||||||||||||||||||||||
| Q690FT | D | 0.20 | ≤1.80 | 0.020 | 0.010 | 0.60 | 0.07 | 0.15 | 0.050 | 0.50 | 0.80 | 0.80 | 0.80 | 0.015 | 0.012 | |||||||||||||||||
| E | 0.010 | |||||||||||||||||||||||||||||||
| The lower limit of Mn content for steel plates delivered in normalized condition shall be as specified in Table 1. No lower limit of Mn content shall be required for steel plates delivered in other conditions. | ||||||||||||||||||||||||||||||||
Mechanical properties
| Grade | Quality grade | Transverse yield strength Rel /(N/mm²) ≥ Thickness(mm) |
Tensile strength Rm/(N/mm²) |
Post-fracture growth rate A/% |
Impact power KV2 /J ≥ |
180°Bending test d=bending mandrel diameter a=Sample thickness Thickness |
||||||||||||||||
| ≤16 | >16~40 | >40~100 | ≤16 | >16~100 | ||||||||||||||||||
| Q235FT | B、C、D | 235 | 225 | 215 | 360~510 | 24 | 47 | d=2a | d=3a | |||||||||||||
| E | 34 | |||||||||||||||||||||
| Q275FT | C、D | 275 | 265 | 255 | 410~560 | 21 | 47 | |||||||||||||||
| E、F | 34 | |||||||||||||||||||||
| Q345FT | C、D | 345 | 335 | 325 | 470~630 | 21 | 47 | |||||||||||||||
| E、F | 34 | |||||||||||||||||||||
| Q420FT | C、D | 420 | 400 | 390 | 520~680 | 19 | 47 | |||||||||||||||
| E、F | 34 | |||||||||||||||||||||
| Q460FT | C、D | 460 | 440 | 420 | 550~720 | 17 | 47 | |||||||||||||||
| E、F | 34 | |||||||||||||||||||||
| Q550FT | D | 550 | 530 | 670~830 | 16 | 47 | ||||||||||||||||
| E | 34 | |||||||||||||||||||||
| Q620FT | D | 620 | 600 | 710~880 | 15 | 47 | ||||||||||||||||
| E | 34 | |||||||||||||||||||||
| Q690FT | D | 690 | 670 | 770~940 | 14 | 47 | ||||||||||||||||
| E | 34 | |||||||||||||||||||||
| 1.When yield is not obvious, Rp0.2 can be used instead of lower yield. | ||||||||||||||||||||||
| 2.When the thickness is greater than 60 mm, the elongation after fracture can be reduced by 1%. | ||||||||||||||||||||||
| 3.The impact test used longitudinal specimens. | ||||||||||||||||||||||
| 4.Impact test temperatures corresponding to different quality grades:B—20℃、C—0℃、D— -20℃、E— -40℃、F— -50℃。 | ||||||||||||||||||||||