This series of products is for household appliance steel; the choice of material depends on the specific requirements. Below, we will introduce the thickness range, delivery status, and applicable standards for each grade that we can provide. We hope this information is helpful. If you have any questions about the products or need a quote, please contact us via email. We apologize that some grades may be categorized into multiple types based on their applications, which could make your search inconvenient. We also welcome any suggestions you may have. Thank you very much!
Spot inventory inquiry Spot inventoryIf conditions permit, we can also provide steel mill customization services, where the thickness, width, and length can all be made to your needs, just like a tailor making clothes for you, implementing personalized orders.
Steel mill customized business email: customize@cehesteel.com
Cold-rolled enamel steel supply range
| Implementation Standards | Grade | Product Specifications/mm | Delivery status | Remarks | ||||||||||||||||||||||||
| JIS G3133-2009 | SPP-H | 0.35~2.0×850~1250 0.40~2.0×850~1300 0.50~2.0×850~1340 0.60~2.0×850~1360 0.70~2.0×850~1400 (Thickness 0.70 and above, uncut edge width can reach 1420,limit1430) |
SD | (Thickness 0.70 and above, uncut edge width can reach1420,limit1430) | ||||||||||||||||||||||||
| Q/XGJ288-2019 | XTC4D | |||||||||||||||||||||||||||
| EN10209:2008 | DC01EK DC03EK/DC03ED DCO4EK DC05EK DC06EK/DC06ED |
0.35~2.0×850~1250 0.40~2.0×850~1300 0.50~2.0×850~1340 0.60~2.0×850~1360 0.70~2.0×850~1400 (Without edge cutting when thickness is 0.70 or above,the width can reach up to 1420,limit value:1430) |
(Without edge cutting when thickness is 0.70 or above,the width can reach up to 1420,limit value:1430) | |||||||||||||||||||||||||
| ASTM A424/A424M:2018 | TypeI | |||||||||||||||||||||||||||
Typical product applications
| Grade | Surface grade | Main uses | Deep pressure level | ||||||||||||||||
| DCO1EK | FB | Light industry (gas appliances, cookware), home appliances (ovens, ovens), environmental protection (desulfurization and denitrification equipment). | General stamping | ||||||||||||||||
| FC | Architectural decoration, medical and health care, artistic enamel | ||||||||||||||||||
| DC03EK | FB | Light industry (gas appliances, cookware), home appliances (ovens, ovens), environmental protection (desulfurization and denitrification equipment) |
Deep pressure level | ||||||||||||||||
| FC | Architectural decoration, medical and health care, artistic enamel | ||||||||||||||||||
| DC04EK DC05EK DC06EK |
FB | Light industry (gas appliances, cookware), home appliances (ovens, ovens) | Ultra-deep drawing class | ||||||||||||||||
| FC | Architectural decoration, medical and health care, artistic enamel | ||||||||||||||||||
| XTC4D/SPP-H | FB | Environmental protection (desulfurization and denitrification equipment) | It generally does not require stamping and has a certain degree of bending performance. |
||||||||||||||||
Product mechanical properties and characteristics
| Grade | Implementation Standards | Yield strength/MPa | Tensile strength/MPa | Elongation/% | Features | ||||||||||||||||
| A50 | A80 | ||||||||||||||||||||
| DC01EK | EN10209 | ≤220 | 270~350 | - | ≥36 | 1)It can meet different stamping levels; 2)Excellent welding performance; 3)Excellent resistance to scale bursting; 4)Excellent adhesion performance; 5)Good resistance to pinhole defects. |
|||||||||||||||
| DC03EK/DC03ED | ≤190 | 270~340 | - | ≥37 | |||||||||||||||||
| DCO4EK | ≤180 | 270~340 | - | ≥38 | |||||||||||||||||
| DCO5EK | ≤170 | - | ≥39 | ||||||||||||||||||
| DCO6EK/DCO6ED | ≤160 | - | ≥39 | ||||||||||||||||||
| SPP-H | JISG3133 | - | 270~350 | - | - | ||||||||||||||||
| XTC4D | Q/XGJ288 | 140~240 | 270~340 | ≥35 | - | It has certain bending properties, good resistance to blistering, good adhesion and good resistance to pinholes. | |||||||||||||||
| Grade | Chemical composition (mass fraction)/% | |||||||||||||||||||
| C | Mn | P | S | Alsc | Ti | |||||||||||||||
| DC03EKd | ≤0.08 | ≤0.60 | ≤0.045 | ≤0.045 | ≥0.015 | — | ||||||||||||||
| DC03EKd | ≤0.06 | ≤0.40 | ≤0.025 | ≤0.030 | ≥0.015 | —a | ||||||||||||||
| DC05EK | ≤0.008 | ≤0.25 | ≤0.020 | ≤0.050 | ≥0.010 | ≤0.3b | ||||||||||||||
| a.Elements such as boron can be added; b.Titanium can be replaced by niobium, etc., but carbon and nitrogen should be completely fixed; c.Alt can be used instead; the lower limit of Alt is 0.005% higher than the value specified in the table. d.When the carbon content is no more than 0.008%, the lower limit of Als can be 0.010%. |
||||||||||||||||||||
| Grade | ReL a,b/MPa≤ | Rm/MPa | Elongation after fracture c,dA80mm,%≥ | r90e≥ | n90e≥ | |||||||||||||||||
| DC01EK | 280 | 270~410 | 30 | — | — | |||||||||||||||||
| DC03EK | 240 | 270~370 | 34 | 1.3 | — | |||||||||||||||||
| DC05EK | 200 | 270~350 | 38 | 1.6 | 0.18 | |||||||||||||||||
| a:Rrmo.z is used when there is no obvious yield.When the thickness is greater than 0.50 mm but not greater than 0.70 mm, the upper limit of the yield strength can be increased by 20 MPa; when the thickness is not greater than 0.50 mm, the upper limit of the yield strength can be increased by 40 MPa. b:With the consent of both the supplier and the buyer, the lower limit of the yield strength of DC01EK and DC03EK can be set at 140 MPa, and that of DC05EK can be set at 120 MPa; c:The sample width b is 20 mm, and the sample direction is transverse. d:When the thickness is greater than 0.50 mm and not greater than 0.70 nm, the minimum elongation after fracture can be reduced by 2% (absolute value); when the thickness is not greater than 0.50 mm, the minimum elongation after fracture can be reduced by 4% (absolute value). e:The requirements for r90 and n90 values only apply to products with a thickness of ≤0.50mm. When the thickness is greater than 2.0mm, the r₃ value can be reduced by 0.2. |
||||||||||||||||||||||
Typical enamel steel is sensitive to scale explosion.
| Grade | Hydrogen permeation timetb(min) | Thickness(mm) | Anti-scaling sensitivityTH(min/mm²) | ||||||||||
| XTC4D | 24.00 | 0.66 | 55.10 | ||||||||||
| DC03EK | 11.25 | 0.64 | 26.01 | ||||||||||
| DC03EK | 12.25 | 0.66 | 28.12 | ||||||||||
Deep drawing steel supply range
| Implementation Standards | Grade | Product Specifications/mm | Delivery status | |||||||||||||||
| GB/T5213-2019 EN10130-2006 Q/XGJ222-2021 |
DC03 | 0.3~2.0×850~1100 0.35~2.0×850~1250 0.4~2.0×850~1300 0.5~2.0×850~1340 0.6~2.0×850~1360 0.7~2.0×850~1400 |
Annealing + leveling SB or SD | |||||||||||||||
| DC04 | ||||||||||||||||||
| DC05 | Annealing+ leveling SB or SD | |||||||||||||||||
| Dc06 | ||||||||||||||||||
Mechanical properties of steel for stamping series
| Material Category | Standard number | Grade | Illustrate | |||||||||||
| General use | JIS G3141 | SPCC | Refrigerator and other household appliance casings, oil drums, steel furniture, and other general forming processes | |||||||||||
| EN 10130 | DC01 | |||||||||||||
| JFS A 2001 | JSC270C | |||||||||||||
| stamping grade | JIS G3141 | SPCD | Steel for stamping and forming of home appliances | |||||||||||
| EN 10130 | DC03 | |||||||||||||
| JFS A 2001 | JSC270D | |||||||||||||
| Deep drawing | JIS G3141 | SPCE | Steel for deep drawing forming | |||||||||||
| EN 10130 | DC04 | |||||||||||||
| JFS A 2001 | JSC270E | |||||||||||||
| extra deep drawing | JIS G3141 | SPCF | Steel for extra-deep stamping forming | |||||||||||
| EN 10130 | DC05 | |||||||||||||
| JFS A 2001 | JSC270F | |||||||||||||
| Ultra-deep drawing | JIS G3141 | SPCG | Steel for ultra-deep drawing forming | |||||||||||
| EN 10130 | DC06 | |||||||||||||
| JFS A 2001 | JSC260G | |||||||||||||
| Extra deep drawing | EN 10130 | DC07 | Steel with exceptional deep-drawing properties | |||||||||||
Mechanical properties of steel for stamping series
| Grade | Yield strength ᵃMPa | Tensile strength MPa≥ | Elongation after fracture ᵇ % A80mm ≥ | |||||||||||||||
| Nominal thickness mm | ||||||||||||||||||
| 0.30~<0.50 | 0.50~<0.70 | 0.70~<1.0 | 1.0~<1.6 | ≥1.6 | ||||||||||||||
| DC01ᵈ | 140~260 | 270~410 | 26 | 28 | 30 | 32 | 34 | |||||||||||
| DC03 | 140~220 | 270~370 | 30 | 32 | 34 | 35 | 36 | |||||||||||
| DC04 | 130~200 | 270~350 | 34 | 36 | 38 | 39 | 40 | |||||||||||
| DC05 | 120~180 | 270~330 | 35 | 38 | 40 | 40 | 41 | |||||||||||
| DC06 | 110~170 | 260~330 | 37 | 39 | 41 | 42 | 43 | |||||||||||
| DC07 | 100~150 | 250~310 | 40 | 42 | 44 | |||||||||||||
| a.Use Rp0.2 if there is no obvious yield point,otherwise, use ReL ,When the thickness is greater than 0.50mm ,And not greater than 0.70mm ,The specified yield strength value may be increased by 20 MPa. When the thickness is no greater than 0.50mm ,The specified yield strength value is allowed to be increased by 40 MPa. |
||||||||||||||||||
| b.The specimen is P6 specimen in GB/T 228, and the specimen orientation is transverse. | ||||||||||||||||||
| d.The upper limit of the yield strength of DC01 is only applicable within 8 days from the date of completion of product manufacturing. | ||||||||||||||||||